Processing Machinery 3 Aufrufe

Poor LDPE Film Transverse Tear

Problembeschreibung
The transverse tear strength is significantly lower than the longitudinal, with unbalanced performance.
Ursachenanalyse
An insufficient blow-up ratio leaves the transverse molecular chains not fully extended; uneven die output also scatters transverse performance.; During on-site troubleshooting, verify item by item according to this mechanism, and avoid blindly adjusting the machine based only on experience.
Lösung
①Increase the blow-up ratio to 2~4 times; ②Balance biaxial stretching; ③Check die uniformity; ④A small amount of LLDPE can be added to improve overall strength.; After adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability.
Wichtigste Erkenntnis
Transverse-longitudinal balance is the basic goal of film design; blow-up ratio adjustment combined with resin modification can quickly correct the imbalance.; After confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
LDPE; film; transverse tear; blow-up ratio; LLDPE; balance