【Problem phenomenon】When plasticizing PVDF with high back pressure, the actual melt temperature exceeds the set value, and products discolor and lose strength
Ursachenanalyse
PVDF is shear-sensitive; shear heat generated by high back pressure and high screw speed superimposes on external heating, making the actual melt temperature exceed the limit; the CS-Seal guide explicitly specifies low back pressure to prevent shear heat accumulation
Lösung
Take a low back pressure value and reduce screw speed; calibrate settings based on measured melt temperature; when plasticization is insufficient, prioritize raising external heat rather than adding shear; After adjustment, take consecutive samples to verify the effect, and resume mass production only after confirming stability
Wichtigste Erkenntnis
Shear heat is an invisible overtemperature source; PVDF requires low back pressure and low screw speed for plasticization; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence; Include this case in the defect archive as a reference for troubleshooting similar problems in the future