Poor interfacial bonding between EAA and filler
Problembeschreibung
The tensile strength of the EAA/filler composite is lower than that of pure EAA, playing a negative role
Ursachenanalyse
Poor interfacial affinity between filler and EAA, no coupling agent treatment used; filler particles agglomerate, dispersed particle size >5μm; EAA has insufficient wettability to rigid fillers
Lösung
1) Pretreat the filler with silane coupling agent KH-560 at 0.5-1wt%; 2) Add 2-3wt% EAA compatibilizer to strengthen interfacial bonding; 3) Use ultrafine filler d50<2μm; 4) Twin-screw high-shear blending to ensure dispersion
Wichtigste Erkenntnis
The elastomer-filler interface requires the dual action of coupling agent and compatibilizer, otherwise the filler has a negative effect