Glass Fibre surface orange peel texture

Problembeschreibung
Glass Fibre product surface orange-peel-like uneven texture, feels rough
Ursachenanalyse
Mold temperature too low <30°C, product surface rapidly cools and solidifies, then interior continues shrinking causing surface unevenness; injection speed too low
Lösung
1) Raise mold temperature to 40-50°C to delay surface solidification; 2) appropriately raise injection speed; 3) increase holding pressure to reduce internal shrinkage
Wichtigste Erkenntnis
Orange peel texture is caused by rapid cooling and solidification; raising mold temperature and holding pressure are key
Glass Fibreorange peel texturemold temperatureholding pressuresurface solidification