Fiber exposure in PET reinforced material
Problembeschreibung
Glass fiber is exposed on the surface of glass fiber reinforced PET injection molded products, with a rough hand feel and uneven color.
Ursachenanalyse
Mold temperature is on the low side; the melt surface layer cools quickly and the glass fiber cannot be fully covered; injection speed is on the slow side; glass fiber content is on the high side.
Lösung
Increase mold temperature to 140-160°C; increase injection speed (fast filling); reduce glass fiber content or use chopped glass fiber.
Wichtigste Erkenntnis
The surface quality of PET reinforced products depends on high-temperature molds and fast filling.