Extrusion & Post 9 Aufrufe

Extruded PEEK pipes crack due to large internal stress

Problembeschreibung
Extruded pipes/rods crack on their own after placement
Ursachenanalyse
Cooling too fast after extrusion causes a temperature difference between the surface layer and the core, producing quenching stress; the volume effect of PEEK crystallization shrinkage; inconsistent internal and external cooling rates
Lösung
Use segmented gradient cooling (hot→warm→cold) instead of direct cooling; post-anneal the product at 250°C/2h to eliminate stress; control the matching of extrusion speed and cooling speed
Wichtigste Erkenntnis
Annealing treatment is the most effective method to eliminate internal stress in PEEK products
internal stressannealinggradient coolingcrackingextrusion