Molds & Tooling 7 조회수

ASA improper mold temperature poor gloss

문제 현상
ASA product surface gloss is low, dark and matte, not matching exterior high-gloss requirements; after raising mold temperature, cycle extends but gloss improvement is limited.
원인 분석
Mold temperature directly affects ASA surface replication and rubber phase distribution state; 30~60℃ mold temperature suits general parts, high-gloss appearance parts need a higher mold temperature range; insufficient cavity polishing also limits the gloss upper limit.
해결 방법
①Raise mold temperature of high-gloss parts to 60~80℃ and verify surface improvement; ②mirror polishing of cavity to high-gloss standard; ③cooperate with higher melt temperature and injection speed; ④balance gloss and cycle by optimizing cooling water channels.
핵심 요약
ASA gloss is the superposition of three elements: mold temperature, polishing, and temperature-speed; mold polishing investment for exterior parts cannot be saved; the contradiction between cycle and gloss is reconciled by water channel optimization.
ASA; gloss; mold temperature; polishing; appearance; high gloss