Molds & Tooling 3 조회수

EVA Foaming Uneven Expansion Ratio

문제 현상
The density difference of foamed products from the same mold exceeds 15%, and the mechanical properties fluctuate greatly.
원인 분석
A mold temperature difference greater than 10℃ makes the local decomposition rate of the foaming agent different (AC foaming agent decomposition temperature 160~200℃); incomplete crosslinking with residual crosslinking agent exceeding 10% also causes shrinkage rate fluctuations.
해결 방법
①Optimize the mold heating channel design; ②adopt a high-precision temperature control system with an error of ±1℃; ③increase the vulcanization temperature to 170~180℃ and add accelerators such as magnesium oxide; ④test the foaming agent decomposition curve for each batch.
핵심 요약
Foaming ratio uniformity is determined by mold temperature consistency and crosslinking sufficiency; temperature control accuracy and additive batch management are the two handles.; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
EVA; foaming; expansion ratio; mold temperature; crosslinking; foaming agent