Extrusion & Post
4 조회수
LLDPE blown film die lip buildup
문제 현상
Die lip buildup gradually increases, requiring frequent shutdowns for cleaning, and streaks appear on the film surface.
원인 분석
LLDPE high-viscosity melt easily adheres and accumulates at stress concentration points on the die exit wall; antiblock agents and other additives also accelerate precipitation and buildup.; During on-site troubleshooting, verify item by item according to this mechanism, avoiding blindly adjusting the machine based only on experience.
해결 방법
①Add 300ppm-level PPA aid to form a die wall lubricating layer; ②regularly clean the die exit; ③optimize die exit temperature; ④evaluate additive precipitation effects.; After adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability.
핵심 요약
Die lip buildup is a persistent problem in LLDPE production; PPA lubricating layer technology can significantly extend the die cleaning cycle.; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence.
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다
의견 주셔서 감사합니다!