Extrusion & Post 4 조회수

LLDPE blown film sharkskin

문제 현상
Periodic ripples like sharkskin appear on the bubble surface, and transparent film loses gloss
원인 분석
LLDPE has high melt fracture sensitivity; too low die temperature or too low resin melt index triggers it; narrow MWD lacks shear thinning, making the critical shear rate lower; when troubleshooting on site, verify item by item according to this mechanism to avoid blindly adjusting the machine based only on experience
해결 방법
①Raise die temperature by 10-20°C; ②switch to high melt index resin; ③add fluoroelastomer processing aid PPA; after adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability
핵심 요약
LLDPE sharkskin is harder to cure than LDPE; raising die temperature, changing melt index and adding PPA often need to be combined; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
LLDPE;sharkskin;melt fracture;die temperature;PPA