Material Drying 4 조회수

PA12 FDM Filament Drying and Clogging

문제 현상
【Problem phenomenon】FDM printing of PA12 filament had nozzle clogging and intermittent extrusion, and printed parts had bubbles and poor layer texture
원인 분석
After PA12 filament absorbs moisture, the moisture vaporizes during printing, clogging the nozzle and forming bubbles; FDM filament must be dried at 60℃ for more than 4 hours, sealed after drying, and exposed for no more than 30 minutes
해결 방법
Dry the filament at 60℃×4h or more and store it sealed; equip dehumidification equipment in environments with humidity greater than 60%; re-dry filament exposed beyond the time limit before putting it on the machine; after adjustment, take consecutive samples to verify the effect, and resume mass production only after confirming stability
핵심 요약
FDM filament is dried at 60℃×4h, sealed for use, and 30 minutes of exposure is the upper limit; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
FDM filamentdryingnozzle cloggingbubbles

이 정보가 도움이 되었나요?

0 명이 도움이 되었다고 합니다