Material Drying 4 조회수

PA6 Hydrolysis Causes Sharp Strength Drop

문제 현상
The product appearance was normal, but impact and tensile strength dropped significantly, breaking after assembly; appearance inspection is hard to find it, which is a hidden failure.
원인 분석
Moisture-containing PA6 undergoes hydrolysis at melting temperature, amide bonds break, and molecular weight declines irreversibly; hydrolysis has no obvious appearance features, but mechanical properties have been seriously damaged, and products break in batches during use, which is extremely harmful.
해결 방법
①Strictly dry to moisture content <0.2%;②verify moisture before startup;③wet material must not be used directly;④use up opened material within 48~72 hours or re-dry it;⑤shorten the residence time of the melt in the barrel to reduce heat accumulation degradation.
핵심 요약
PA6 hydrolysis = 'irreversible invisible killer': products with normal appearance may already be performance-scrapped; drying is PA6's performance insurance, and directly molding wet material is tantamount to delivering scrap to the customer.
PA6; hydrolysis; strength; molecular weight; drying