문제 현상
After changing from PA66 to PA6, the product showed unmelted spots or degradation, with abnormal quality.
원인 분석
The melting points of the two differ by 40℃, and the material change temperature setting was wrong: processing PA66 at PA6 temperature causes poor plasticization, and conversely PA6 overheats and degrades; not switching the temperature system is the root cause.
해결 방법
①For material change, reset the temperature according to the target material and stabilize for 15~20 minutes;②use purging material to thoroughly replace and clean during material change;③fully inspect the first article after material change to confirm thorough replacement;④record and execute the material change cleaning SOP;⑤avoid frequent cross changeover to reduce cross-contamination.
핵심 요약
PA6/PA66 material change = 'temperature system switching': applying parameters is strictly prohibited; the 40℃ melting point difference determines that material change must reset the temperature and thoroughly replace, and cannot seek convenience.
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다
의견 주셔서 감사합니다!