메뉴
재료 기계
인사이트
기사 동영상 문제 및 해결책
About
Chembull 소개 미디어 파트너
문의하기
언어
EnglishالعربيةPortuguêsEspañolDeutschTürkçe한국어
문제 및 해결책으로 돌아가기
Molds & Tooling 3 조회수

PA66 post-crystallization dimensional drift

문제 현상
Dimensions continue to change after low-mold-temperature molding, precision parts out of tolerance.
원인 분석
Insufficient crystallinity at low mold temperature, continued crystallization after demolding; environmental temperature and humidity participate; post-crystallization is an aging characteristic; during on-site troubleshooting, verify item by item according to this mechanism, and avoid blindly adjusting the machine based solely on experience.
해결 방법
①Mold temperature 80~100℃ to lock crystallization; ②extend cooling time so products are fully set before demolding; ③uniformly specify measurement aging (e.g., 24 hours after molding); ④perform annealing when necessary to eliminate residual stress; ⑤stabilize the environment.
핵심 요약
PA66 post-crystallization='insufficient mold temperature': raising mold temperature to lock crystallization is fundamental; manage dimensions after aging, especially guard against low-mold-temperature parts; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence.
PA66; post-crystallization; mold temperature; dimension; aging

이 정보가 도움이 되었나요?

0 명이 도움이 되었다고 합니다