Processing Machinery 3 조회수

PA66 and PA6 temperatures cannot be borrowed from each other

문제 현상
Using PA6's 240-270℃ process to process PA66 causes poor plasticizing and short shots; the reverse causes severe PA6 degradation
원인 분석
PA66 melting point 260℃ is 40℃ higher than PA6, the two melt temperature ranges do not overlap at all; material changeover on the same machine must replace the entire temperature curve, borrowing parameters inevitably leaves one side undercooked and the other overheated
해결 방법
①After material changeover, reset barrel temperatures and stabilize 15-20 minutes before production; ②use HDPE etc. as transition material for thorough purging during changeover; ③archive temperature curves by grade for recall
핵심 요약
PA6 and PA66 are of the same family but different windows; material changeover must change the full set of parameters and fully stabilize, transition-period products are isolated and handled separately; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
PA66; PA6; material changeover; temperature window; stabilization time