PA6 Barrel Purging Temperature
문제 현상
After PA6 production ends, the next material is directly used to push out the residue, and black specks persist for a long time after material change
원인 분석
PA6 melt temperature is high, and residual material carbonizes in the dead corners of the barrel; directly pushing out with new material has low purging efficiency, and carbonized spots fall off one after another forming black specks; when troubleshooting on site, verify item by item according to this mechanism, and avoid blindly adjusting the machine based only on experience
해결 방법
Before shutdown, purge the barrel with purging compound or HDPE at 260°C to completely expel the PA6 residue; purge and cool down before long-term shutdown; disassemble and clean the screw and nozzle to remove accumulated material in dead corners
핵심 요약
High-temperature material shutdown purging must be thorough, and carbonized material in dead corners is the main source of black specks; after confirming effectiveness, fix the parameters and practices into the work instructions to prevent recurrence; include this case in the defect archive as a reference for troubleshooting similar problems in the future
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다
의견 주셔서 감사합니다!