Injection Molding 6 조회수

PC Birefringence (Rainbow Pattern)

문제 현상
Transparent PC parts show rainbow-shaped interference fringes under polarized light, optical parts (lenses, light guides) are unqualified.
원인 분석
Polymer orientation frozen by filling and holding pressure forms internal stress, causing birefringence; high injection speed, high holding pressure, and low-temperature molds all aggravate orientation stress, which appears optically as rainbow patterns.
해결 방법
①Reduce injection speed and holding pressure; ②Increase mold temperature and melt temperature; ③Enlarge the gate to reduce shear; ④Optimize the flow path design for optical parts; ⑤Anneal to eliminate stress when necessary.
핵심 요약
PC rainbow pattern = 'optical development of internal stress': reducing pressure, raising temperature, and annealing can alleviate it; optical parts must minimize orientation stress from flow design, this is more of a design problem than a process problem.
PC; birefringence; rainbow pattern; internal stress; orientation