Material Drying
4 조회수
PC moisture content 0.02% red line
문제 현상
【Problem Phenomenon】PC drying released by experience, moisture content exceeding standard causes silver streaks and brittle fracture
원인 분석
PC is strongly hygroscopic and extremely prone to hydrolysis at high temperature, moisture content must be ≤0.02%; excessive moisture at 280-320℃ causes PC hydrolysis with molecular weight plummeting, appearance silver streaks and impact strength drop occurring simultaneously
해결 방법
Dehumidifying dryer 120℃×3-4h; moisture meter measured ≤0.02% before release; dried material goes directly into the machine to prevent moisture regain;After adjustment, take continuous samples to verify the effect, and resume mass production only after confirming stability
핵심 요약
PC moisture content 0.02% is the life-and-death line, measured release not by experience;After confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence;Include this case in the defect archive as a reference for troubleshooting similar problems in the future
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다
의견 주셔서 감사합니다!