PEEK Cooling Time Far Exceeds Conventional Plastics
문제 현상
[Problem Phenomenon] PEEK parts whose cooling time is set following ABS experience deform at ejection and have unstable dimensions
원인 분석
3mm-wall PEEK needs 60-90 seconds of controlled cooling while ABS only needs 25-35 seconds, because the latent heat released during crystallization must be fully conducted away; insufficient cooling causes ejection deformation and post-crystallization dimensional drift
해결 방법
Set the cooling time according to wall thickness and crystallization needs — start at 60-90 seconds for 3mm walls; include crystallization latent heat in the cooling design; do not optimize the cycle at the cost of crystallization completeness
핵심 요약
PEEK cooling involves crystallization latent heat — doubling the time is normal, do not forcibly compress the cycle; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence; include this case in the defect archive as a troubleshooting reference for similar problems in the future
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다
의견 주셔서 감사합니다!