메뉴
재료 기계
인사이트
기사 동영상 문제 및 해결책
About
Chembull 소개 미디어 파트너
문의하기
언어
EnglishالعربيةPortuguêsEspañolDeutschTürkçe한국어
문제 및 해결책으로 돌아가기
Material Drying 7 조회수

PET Preform Bubbles (Insufficient Drying)

문제 현상
Round bubbles and water-blister-like cavities appear inside or on the surface of transparent preforms; after blowing, the bubble areas are stretched thin and even form pinholes.
원인 분석
PET pellets absorb moisture and the moisture content exceeds the standard; during melting, water vaporizes and induces hydrolysis; drying dew point not meeting standard or insufficient drying residence time is the main cause, and an excessively high regrind ratio also brings in moisture and volatiles.
해결 방법
①Dehumidifying drying 150~180℃×4~6h, moisture content reduced below 50ppm; ②calibrate dryer dew point and air volume; ③reduce the regrind ratio and convey sealed; ④re-dry damped pellets before use.
핵심 요약
Preform bubbles are almost all related to moisture management, and qualified drying is the primary prerequisite; bubbled preforms will inevitably be stretched thin during blowing, so they should be rejected online and the drying records traced, and after confirming the measures are effective, solidify them into the work instruction.
PET; preform; bubble; drying; moisture content; hydrolysis

이 정보가 도움이 되었나요?

0 명이 도움이 되었다고 합니다

ChemAI