Material Analysis 11 조회수

PP Part Low-temperature Drop Fracture

문제 현상
PP turnover boxes and containers fracture at corners on drop in winter or low-temperature environments, yet pass tests at room temperature.
원인 분석
Homopolymer PP has poor low-temperature toughness; stress concentration areas like corners crack brittlely more easily at low temperature; weld lines passing through corners further weaken them; improper grade selection is the root cause.
해결 방법
①Select impact copolymer PP grades for low-temperature use; ②add fillets and reinforcing ribs at corners to eliminate stress concentration; ③avoid weld lines passing through stressed areas like corners; ④perform drop verification under actual low-temperature environment; ⑤if necessary, switch to more low-temperature-resistant materials.
핵심 요약
For PP low-temperature drop fracture, first modify the structure (fillets, reinforcing ribs, weld line avoidance), then change the grade (impact copolymer); passing at room temperature does not mean passing at low temperature—verification must simulate real use temperature.
PP;low temperature;drop;copolymer;fillet;grade