Material Drying 4 조회수

PVDF Thick-Walled Rod Internal Bubbles and Voids

문제 현상
【Problem phenomenon】Concentrated bands of bubbles and voids appear in the cross-section of PVDF thick-walled rods, exposed after machining
원인 분석
Thick-walled rods cool slowly and have long compensation paths, so residual moisture, gas, and shrinkage voids concentrate in the core; insufficient raw '2079851475616104451 and excessive injection speed entraining air superimpose and aggravate
해결 방법
Dry the raw material at 80-100℃×2-4h to below 0.05% moisture; reduce injection speed to prevent air entrapment; stage and extend holding pressure for compensation; design rod molds with sufficient cooling and compensation channels
핵심 요약
Core defects of thick-walled rods originate from insufficient drying plus inadequate compensation; treat both causes together; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence; Include this case in the defect archive as a reference for troubleshooting similar problems in the future