Poor weather resistance of EAA
문제 현상
After 6 months outdoors, the mechanical properties of EAA decrease by 40-50%, surface cracking
원인 분석
The polyolefin backbone of EAA undergoes photo-oxidative degradation, molecular chains break; ultraviolet rays directly attack C-C bonds
해결 방법
1) UV-327 0.5-1wt% to absorb ultraviolet rays; 2) HALS-770 0.2-0.5wt% for light stabilization; 3) 1010+168 antioxidant 0.3wt% to prevent oxidation
핵심 요약
Poor weather resistance is caused by photo-oxidation; UV+HALS+antioxidant triple protection is the key