Molding Process
7 조회수
EVA extruded film thick at edges and thin in middle
문제 현상
EVA extruded film edges 20-30% thicker than middle with U-shaped thickness distribution
원인 분석
Improper die flow channel design with low edge resistance and large flow; EVA melt elasticity with greater swell at edges; air ring cooling with different edge effect
해결 방법
1) Adopt coat-hanger design for die to balance resistance between middle and edges; 2) Fine-tune die gap slightly larger in middle and slightly smaller at edges for compensation; 3) Slightly reduce air ring edge air volume; 4) Add restrictor bar to adjust edge flow
핵심 요약
U-shaped thickness is caused by die flow channel and swell differences; coat-hanger die and gap fine-tuning are key