Extrusion & Post
10 조회수
Weak Interfacial Adhesion in EVOH Coextrusion
문제 현상
EVOH/PE coextrusion interface adhesion <1N/15mm with delamination
원인 분석
EVOH is highly polar while PE is non-polar, interfacial adhesion is extremely low; no tie layer used
해결 방법
1) Set a tie layer between EVOH and PE (PE-g-MAH or EAA 5-10μm); 2) Coextrusion temperature ensuring full diffusion of the tie layer; 3) Increase tie layer thickness to 8-15μm
핵심 요약
EVOH/PE interface polarity difference is large; a tie layer must be used to solve it