Molds & Tooling 4 조회수

Obvious depressions at thick-wall areas of the product (rib roots, back of bosses)

문제 현상
Obvious depressions at thick-wall areas of the product (rib roots, back of bosses), uneven surface, especially obvious under side light
원인 분석
Holding pressure insufficient or holding time short Gate too small, freezing too early, holding pressure cannot be transmitted Uneven wall thickness, thick-wall areas cool slowly and shrink more Mold temperature on the high side (exceeding the 40-80°C upper limit), slow cooling Melt temperature too high, large volume shrinkage
해결 방법
Increase holding pressure 80-120MPa, hold 15-30s Increase gate cross-sectional area, gate thickness ≥60% of wall thickness Lower mold temperature to the low side of 40-80°C to accelerate cooling Appropriately lower barrel temperature to reduce volume shrinkage Optimize wall thickness design to reduce abrupt changes
핵심 요약
Shrinkage depressions need improvement from the three aspects of holding pressure, gate and mold temperature
sink markholding pressuregatemold temperature