CEF injection flash severe
문제 현상
The parting line flash of the CEF injection molded part is 0.05-0.1mm, width >2mm, requiring secondary trimming
원인 분석
The injection pressure is too high >80MPa and the melt overflows from the parting line; the clamping force is insufficient; the mold parting line fitting gap is >0.02mm
해결 방법
1) Reduce the injection pressure to 60-70MPa; 2) Increase the clamping force or use a larger tonnage '2079851475616104452 machine; 3) Mold fitting gap <0.02mm; 4) Increase the melt viscosity to reduce the tendency of mold seepage
핵심 요약
Flash is caused by high-pressure injection and mold gap; reducing pressure and improving mold fitting are the key
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다
의견 주셔서 감사합니다!