Extrusion & Post
4 조회수
POE extrusion pipe inner wall rough
문제 현상
POE extruded pipe inner wall roughness Ra>10μm, affecting fluid conveying efficiency
원인 분석
Mandrel surface rough or worn; insufficient internal cooling causes inner wall melt not fully sized; POE melt elasticity causes uneven die swell of the inner wall
해결 방법
1) Polish mandrel to Ra<0.4μm; 2) Optimize internal cooling system, pass cooling water through the mandrel; 3) Reduce extrusion rate to reduce elastic recovery influence; 4) Add a small amount of low-elasticity resin to improve inner wall smoothness
핵심 요약
Pipe inner wall roughness is caused by mandrel condition and insufficient cooling; polishing mandrel and internal cooling are key
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다