Extrusion & Post 4 조회수

Metallocene linear low density polyethylene blown film wrinkles

문제 현상
Longitudinal wrinkles appear in the film during hauling, affecting film flatness and subsequent processing. The wrinkles become more obvious after winding, and in severe cases cause the film to be scrapped.
원인 분석
(1) Film thickness uneven, thin parts shrink first producing wrinkles\ (2) Haul-off roll pressure uneven\ (3) Collapsing frame angle improper or the included angle asymmetric\ (4) Cooling line height unstable\ (5) Uneven cooling at various parts of the film causes different shrinkage
해결 방법
(1) Adjust the die gap and air ring, ensure uniform film thickness\ (2) Adjust the haul-off roll pressure, ensure uniform clamping\ (3) Adjust the collapsing frame angle symmetrically, generally an included angle of 30-45°\ (4) Stabilize the cooling line height, fluctuation not exceeding ±50mm\ (5) Check the air ring cooling uniformity, replace with a high-efficiency air ring if necessary
핵심 요약
Wrinkles are caused by uneven thickness or unbalanced hauling, and need to be solved from thickness control, hauling and collapsing frame adjustment.
film wrinklesuneven thicknesshaul-off rollscollapsing framecooling line