Extrusion & Post 11 조회수

Thermal Aging Performance of Polypropylene PPR Pipe Not Up to Standard

문제 현상
After thermal aging, the mechanical properties of PPR/PP-R pipes decline significantly, and the oxidation induction time is insufficient. Thermal aging performance not up to standard shortens the service life of the pipe, and is especially critical in hot water systems.
원인 분석
(1) The antioxidant content of the raw material is insufficient or the type is improper (2) The extrusion temperature is too high, and the antioxidant decomposes and is consumed (3) Too much regrind is used, and the antioxidant content is low (4) The service temperature of the pipe exceeds the design temperature (5) The amount of heat stabilizer added is insufficient to meet the 110°C test requirement
해결 방법
(1) Select a PPR special material containing sufficient antioxidants (2) Control the extrusion temperature at 200-220°C to avoid thermal decomposition of antioxidants (3) Control the regrind ratio to not exceed 15% (4) Ensure the hot water system temperature is within the design range (generally 70°C water supply) (5) Add a combination of hindered phenolic and phosphite antioxidants when necessary
핵심 요약
Thermal aging performance not up to standard is caused by an insufficient antioxidant system, and needs to be solved from formulation and processing temperature control.
thermal agingantioxidantPPRoxidation induction timeextrusion temperature

이 정보가 도움이 되었나요?

0 명이 도움이 되었다고 합니다

ChemAI