Product dense silver streaks/bubbles
문제 현상
Large areas of silver streaks and tiny bubbles appear on PEI injection molded products
원인 분석
Insufficient drying with moisture content >0.05% (PEI saturated water absorption 1.25%, requires 150°C/4-6h drying); processing temperature too high exceeding the safe window (>400°C), causing decomposition and gas generation
해결 방법
Strictly implement 150°C/4-6h drying to make moisture content <0.02%; control the maximum melt temperature ≤390°C; increase back pressure to extrude gas
핵심 요약
The strong hygroscopicity of PEI (1.25%) is the main cause of silver streaks and bubbles