Molding Process
5 görüntüleme
HDPE Sink Mark and Holding Pressure
Sorun Belirtisi
Sink marks are obvious on the back of product reinforcing ribs, with depressions at wall thickness intersections
Neden Analizi
HDPE high shrinkage makes thick-wall areas demand large shrinkage compensation; insufficient holding pressure or time forms sink marks; rib backs are high-incidence positions for sink marks, aggravated when rib thickness exceeds 60% of main wall thickness
Çözüm
①Increase holding pressure and time; ②rib thickness ≤60% of main wall thickness; ③arrange the gate near thick-wall areas; after adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability
Temel Çıkarım
HDPE sink mark treatment emphasizes both holding pressure and structure; rib design is the first line of defense against sink marks; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
Bu faydalı oldu mu?
0 kişi bunu faydalı buldu
Geri bildiriminiz için teşekkürler!