Material Drying 4 görüntüleme

PC/ABS insufficient drying silver streak

Sorun Belirtisi
Silver-white streaks appear on the part surface, distributed in a U-shaped fan near the gate.
Neden Analizi
PC/ABS is highly hygroscopic; when the moisture content exceeds the standard, the moisture vaporizes into steam during '2079851475616104452 and is sheared at the gate to form U-shaped silver streaks; incomplete drying is the most common cause of silver streaks.
Çözüm
①Dehumidification drying at 100~110℃ for 3~4 hours; ②reduce moisture content to below 0.02%; ③check the dryer dew point and motor rotation direction to confirm real drying; ④sealed conveying after drying.
Temel Çıkarım
90% of PC/ABS silver streaks originate from drying; do not judge dryness by the appearance of the pellets, the moisture content must be measured before adjusting the machine.; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
PC/ABS;drying;silver streak;moisture content;dew point;hydrolysis