Injection Molding 12 görüntüleme

PMMA Stress Cracking

Sorun Belirtisi
Products crack during assembly, solvent contact or after storage, often starting from sharp corners and screw bosses.
Neden Analizi
PMMA is brittle and sensitive to residual stress; high stress from fast injection, cold demolding, sharp corners and press fits cracks under solvent or load.
Çözüm
①Slow injection; ②Sufficient cooling and gentle demolding; ③Change sharp corners to rounds (25%~60% of wall thickness); ④Anneal at 70~80℃ for 2~4 hours; ⑤Avoid contact with incompatible solvents.
Temel Çıkarım
PMMA delayed cracking = the delayed detonation of internal stress, annealing is the insurance.
PMMA; stress cracking; annealing; sharp corners; solvents

Bu faydalı oldu mu?

0 kişi bunu faydalı buldu