Processing Machinery 4 görüntüleme

PPS barrel segmented temperature

Sorun Belirtisi
Uneven plasticization causes cloud patterns on products, or excessive front-section temperature causes nozzle drooling and stringing
Neden Analizi
PPS barrel segmentation: rear section about 270-290℃, middle section 300-320℃, front section 300-320℃, nozzle 290-320℃; too high rear section causes pellet bridging, too high front section causes drooling
Çözüm
①Barrel rear section 270-290℃, middle and front sections 300-320℃; ②nozzle 290-320℃ independently controlled; ③hopper seat cooling to prevent bridging
Temel Çıkarım
PPS barrel temperature gradient must balance bridging prevention and drooling prevention; independent nozzle temperature control is the key at the end of the temperature chain; After confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
PPS; barrel temperature; segmentation; nozzle; bridging