Material Drying
5 görüntüleme
PSU Hopper Drying System Requirements
Sorun Belirtisi
[Problem Phenomenon] Hopper-dried PSU repeatedly exceeds moisture content limits; drying effect is unstable
Neden Analizi
Hopper drying requires full insulation and minimal system leakage: inlet air temperature must be high enough to maintain pellet temperature at least 135°C, inlet air dew point -40°C; poor insulation or air leakage collapses drying efficiency
Çözüm
Insulate the hopper and piping and check sealing; monitor inlet air temperature and dew point for compliance; measured pellet temperature above 135°C counts as effective drying; after adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability
Temel Çıkarım
Hopper drying depends on pellet temperature 135°C and dew point -40°C; insulation and air leakage are hidden wounds; After confirming effectiveness, solidify the parameters and practices into the work instructions to prevent recurrence
Bu faydalı oldu mu?
0 kişi bunu faydalı buldu
Geri bildiriminiz için teşekkürler!