Sorun Belirtisi
When EAA is blended with polar resins such as PA/ABS, the extrudate is completely delaminated and the mechanical properties are extremely poor
Neden Analizi
The polarity difference between EAA and polar resins is large, compatibility is zero, interfacial adhesion is extremely low, no compatibilizer is used
Çözüm
1) Use EAA grafted compatibilizer EAA-g-MAH 2-5wt%; 2) Add 1-2wt% epoxy compatibilizer; 3) EAA addition <10wt% to keep the other resin as the continuous phase; 4) Twin-screw high-shear blending to disperse EAA to <0.3μm
Temel Çıkarım
Blends with large polarity differences require reactive compatibilizers to form chemical bonding at the interface to solve the problem
EAA blend delamination polarity difference EAA-g-MAH reactive compatibilization interfacial bonding

Bu faydalı oldu mu?

0 kişi bunu faydalı buldu

ChemAI