Injection Molding 6 görüntüleme

Warpage in EAA '2079851475616104452

Sorun Belirtisi
EAA injection molded products warp 2-3mm/100mm after demolding, flatness does not meet the standard
Neden Analizi
EAA has large shrinkage and uneven mold temperature causes anisotropic shrinkage differences; improper gate position, uneven release of flow orientation stress; insufficient cooling time
Çözüm
1) Raise the mold temperature to 40-60°C to reduce temperature difference; 2) Increase the holding pressure to 50-70MPa; 3) Optimize the gate position to make the flow uniform; 4) Extend the cooling time; 5) Anneal to release residual stress
Temel Çıkarım
Warpage is caused by shrinkage differences and orientation stress; uniform mold temperature and holding pressure are the key
EAA injection warpage shrinkage holding pressure annealing treatment