Injection Molding 6 görüntüleme

Flow marks in EAA '2079851475616104452

Sorun Belirtisi
Radial flow marks centered on the gate appear on the surface of EAA injection molded products
Neden Analizi
Injection speed too fast causes unstable melt front; mold temperature too low <30°C, the front cools rapidly and forms marks
Çözüm
1) Use multi-stage injection speed slow-fast-slow to control front stability; 2) Raise the mold temperature to 40-50°C to delay front cooling; 3) Stabilize the injection pressure to avoid fluctuations; 4) Enlarge the gate area to reduce sudden pressure changes at the gate
Temel Çıkarım
Flow marks are caused by unstable injection front and rapid cooling; multi-stage injection and high mold temperature are the key
EAA injection flow mark injection speed mold temperature gate area