Injection Molding 4 görüntüleme

EEA '2079851475616104452 demolding difficulty

Sorun Belirtisi
EEA injection molded products with large demolding force, products deformed or scratched, demolding time accounting for 30% of the cycle
Neden Analizi
Large adhesion between EEA and the mold cavity; insufficient draft angle <0.5°; insufficient cooling time, product not fully solidified before demolding; unreasonable ejection mechanism design
Çözüm
1) Increase mold draft angle to 1-2°; 2) Extend cooling time so the product is fully solidified before demolding; 3) Polish the mold surface to Ra<0.2μm; 4) Increase ejection area using a large-area ejector plate; 5) Spray release agent (temporary solution)
Temel Çıkarım
Demolding difficulty is caused by adhesion and insufficient mold design; increasing draft angle is the fundamental measure
EEA injectiondemolding difficultydraft angleadhesionejection design

Bu faydalı oldu mu?

0 kişi bunu faydalı buldu

ChemAI