Extrusion & Post
13 görüntüleme
Rough inner wall of EEA extruded pipe
Sorun Belirtisi
EEA extruded pipe inner wall roughness Ra>10μm affecting fluid transport efficiency
Neden Analizi
Mandrel surface rough or worn; insufficient internal cooling causing inner wall melt not fully sized; EEA melt elasticity causing uneven extrusion swell of the inner wall
Çözüm
1) Polish the mandrel to Ra<0.4μm; 2) Optimize the internal cooling system, pass cooling water through the mandrel; 3) Reduce extrusion rate to reduce elastic recovery influence; 4) Add a small amount of low-elasticity resin to improve inner wall smoothness
Temel Çıkarım
Rough pipe inner wall is caused by mandrel condition and insufficient cooling; polishing the mandrel and internal cooling are the key
Bu faydalı oldu mu?
0 kişi bunu faydalı buldu