Injection Molding 6 görüntüleme

EEA Surface Tiger-Skin Stripes

Sorun Belirtisi
Tiger-skin stripes on the surface of EEA injection molded products, alternating light and dark stripes 2-5mm wide
Neden Analizi
Unstable injection speed, melt front fluctuating fast and slow; mold temperature low <30°C, front cools rapidly
Çözüm
1) Multi-stage injection slow-fast-slow to stabilize the front; 2) Increase mold temperature to 40-50°C; 3) Increase injection pressure to stabilize advancement
Temel Çıkarım
Tiger-skin stripes are caused by unstable injection front; multi-stage injection and high mold temperature are key
EEA tiger-skin stripes injection speed multi-stage injection mold temperature control