Material Drying
5 görüntüleme
Silver streaks caused by moisture in EVA processing
Sorun Belirtisi
White silver streak marks appear on EVA injection molded product surface
Neden Analizi
Raw material moisture >0.05% vaporizes during high temperature processing forming bubbles stretched into silver streaks; insufficient drying or hopper condensed water vapor
Çözüm
1) Dry raw material at 80°C for 3-4h to moisture <0.02%; 2) Increase back pressure 0.5-1MPa for venting; 3) Reduce injection speed to avoid air entrapment; 4) Heat hopper to prevent condensed water vapor
Temel Çıkarım
Silver streaks are caused by moisture vaporization and stretching; drying and venting are the main countermeasures