Injection Molding 6 görüntüleme

EVA surface tiger-skin pattern

Sorun Belirtisi
EVA injection molded product surface has tiger-skin pattern with alternating light and dark stripes 2-5mm wide
Neden Analizi
Unstable injection speed with melt front fluctuating fast and slow; mold temperature too low <30°C with the front cooling rapidly
Çözüm
1) Multi-stage injection slow-fast-slow to stabilize the front; 2) Increase mold temperature to 40-50°C; 3) Increase injection pressure for stable advancement
Temel Çıkarım
Tiger-skin pattern is caused by unstable injection front; multi-stage injection and high mold temperature are key
EVA tiger-skin pattern injection speed multi-stage injection mold temperature control