Extrusion & Post 11 görüntüleme

Wrinkling of PU extruded film after winding

Sorun Belirtisi
Transverse wrinkles and longitudinal creases appear after PU extruded film is wound
Neden Analizi
Film tension uneven with fluctuation of ±20%; uneven film thickness causes inconsistent stretching of each section; shrinkage after cooling differs in each direction
Çözüm
1) Automatic tension control system stabilizes winding tension; 2) Improve film thickness uniformity to ±5%; 3) Adjust guide roller parallelism <0.05mm/m; 4) Wind after the film is fully cooled to <30°C
Temel Çıkarım
Film wrinkling is caused by tension fluctuation and uneven thickness; automatic tension control and homogenization are key
PU film winding wrinkling tension control thickness uniformity guide roller parallelism