Extrusion & Post
11 görüntüleme
CEF film printing adhesion poor
Sorun Belirtisi
After printing on the CEF film, the ink adhesion is <2 grade, and large areas fall off in the cross-cut test
Neden Analizi
The polarity of the CEF surface has poor affinity with the ink; the corona treatment effect decays quickly; the ink system does not match CEF
Çözüm
1) Print immediately after corona treatment, within 24h; 2) Use CEF special ink; 3) Increase the corona power to 15-20kW/m² to ensure the surface tension >42mN/m; 4) Flame treatment to assist surface polarization
Temel Çıkarım
Poor printing adhesion is caused by insufficient surface polarity; corona treatment and special ink are the key