Injection Molding
6 görüntüleme
Sink Marks in CMC '2079851475616104452
Sorun Belirtisi
Surface depression of 0.2-0.5mm in thick-walled areas of CMC injection molded products (sink marks)
Neden Analizi
Holding pressure is insufficient or holding time is short; gate freezes prematurely and holding pressure cannot be transmitted; wall thickness difference is large, and after the thin wall freezes, the thick wall cannot be fed
Çözüm
1)Increase holding pressure 70-90MPa; 2)Extend holding to gate freezing +2s; 3)Product design reduces wall thickness differences with gradual transitions; 4)Add supplementary gates in thick-walled areas
Temel Çıkarım
Sink marks are caused by insufficient holding and wall thickness differences; high-pressure holding and multiple gates are core countermeasures