Injection Molding
6 görüntüleme
Glass Fibre injection mold venting burnt
Sorun Belirtisi
Glass Fibre injection mold venting insufficient, air in cavity compressed and heated causing local burning
Neden Analizi
Mold vent groove area insufficient or position improper; injection speed too fast, air has no time to escape; air compressed to high temperature >200°C causing oxidative burning
Çözüm
1) Increase vent groove area, depth 0.02-0.03mm, width 5-10mm; 2) vent grooves set at last-fill region of melt; 3) reduce injection speed to reduce air compression; 4) multi-stage injection with slow advance for venting
Temel Çıkarım
Burning is caused by insufficient venting and high-speed injection compressing air; increasing venting and reducing speed are key
Bu faydalı oldu mu?
0 kişi bunu faydalı buldu
Geri bildiriminiz için teşekkürler!