MP extrusion dimensional instability

Sorun Belirtisi
MP extruded product cross-section dimensions fluctuate ±10%, with periodic variation in the length direction as well
Neden Analizi
feeding amount unstable, feed screw speed fluctuates; extrusion temperature periodically fluctuates ±5°C; haul-off speed mismatched with extrusion speed
Çözüm
1) use a loss-in-weight feeder to ensure stable feeding; 2) PID control of each extruder zone temperature with accuracy ±1°C; 3) closed-loop control of haul-off speed linked with extrusion speed; 4) control processing temperature at 150-170±5°C
Temel Çıkarım
extrusion dimensional stability depends on feeding accuracy, temperature control and haul-off synchronization
MP extrusion dimensional stability feeding control temperature PID haul-off synchronization