Sorun Belirtisi
MP product surface has orange-peel-like uneven texture, rough to the touch
Neden Analizi
mold temperature low <30°C, product surface rapidly cools and solidifies while the interior continues to shrink, causing surface unevenness; injection speed too low
Çözüm
1) raise mold temperature to 40-50°C to delay surface solidification; 2) appropriately increase injection speed; 3) increase holding pressure to reduce internal shrinkage
Temel Çıkarım
orange peel texture is caused by rapid cooling and solidification; raising mold temperature and holding are key